U-Mo and U-Zr alloys - Chemical etching

Material Name: U-Mo and U-Zr alloys
Recipe No.: 10907
Primary Chemical Element in Material: U
Sample Type: Bulk
Uses: General microstructure
Etchant Name: None
Type (Macro/Micro): Micro
Etching Method: Chemical
Etchant (Electrolyte) Composition: 40 ml glycerol, 40 ml HNO3, 10 ml HF.
Procedure (Condition): Immerse or swab sample 5-10 s.
Note: Radioactive metals and alloys.
Reference: Vander Voort, Metallography Principles and Practice, McGraw-Hill, Inc., 1984, p. 675.