10CrMo9-10 Steel

Steel name: 10CrMo9-10
Diagram No.: 5111
Type of diagram: TTP
DIN designation: 10CrMo9-10
Mat. No. (Wr. Nr.) designation: 1.7380
AISI/SAE designation: A182 F22
AFNOR designation: 12CD910
GOST designation: 12Ch8
BS designation: 622/B3
Chemical composition in weight %: 0.08 - 0.14% C, max. 0.50% Si, 0.40-0.80% Mn, max. 0.020% P, max. 0.010% S, 2.00 - 2.50% Cr, 0.90-1.20% Mo, max. 0.012% N, max. 0.30% Cu
Steel group: Alloy special steels
Note: After cooling in air from 950°C the microstructure is bainitic. On tempering above 500 °C the cementite of the bainite is dissolved in under 1000 h. In its place, M2X is precipitated in the form of needles, as described above. Later the carbides M2 C6 and M6C are formed, the former predominating at temperatures around 550°C and the latter at 600°C.
After the usual technical heat treatment 950°C 30 min/air + 750°C 2 h/air, the cementite has been completely dissolved. Instead the carbides M2X and M23C6 and, in the presence of vanadium as impurity, face-centred MX are formed. In addition, M6C is formed on tempering for long times or at higher temperatures.
After transformation with slow cooling from 950 to 650°C in 12 h followed by cooling in air, M2X is found in the microstructure in the form of needles and eutectoid borders. During the subsequent long-time tempering first M23C6 and then M6C is precipitated.
Finally we consider the precipitation behaviour after isothermal transformation (700°C 1 h). In the initial condition M2 X, in the form of needles and eutectic borders, and M23C6 are present. During long-time tempering M6C is precipitated as a further carbide phase, whilst M23C6 is dissolved. It may therefore be assumed that in the steel 10CrMo9-10 only M6C and perhaps also M2X occur as stable carbide phases. Cementite (M3C) and the chromium carbides M7C3 and M23C6 occur only as metastable intermediate phases.
Reference: Not shown in this demo version.

Transformation Diagrams

Price: 20.00 US $
Buy Online Transformation Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagram Calculating Service
CCT and TTT Diagrams Home
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Tempering Diagrams of Steels
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2024 by Steel Data. All Rights Reserved.