CPM REX 76 Steel

Steel name: CPM REX 76
Diagram No.: 1765
AISI/SAE designation: M48
Chemical composition in weight %: 1.50% C, 0.30% Si, min. 0.30% Mn, min. 0.060% S, 3.75% Cr, 5.25% Mo, 3.10% V, 9.75% W
Steel group: PM high speed steels
Properties: No data
Applications: Broaches, end mills, forming tools, hobs, milling cutters, shaper cutters, taps - special, tool bits.
Reference: Not shown in this demo version.

Heat Treatment
Hardening: 2100-2190° F/salt, oil or atmosphere quench to 1000-1100° F, equalize and then air cool to below 125° F or hand warm. Vacuum or atmosphere quench rate through 1850-1300° F range critical to achieve optimum heat treat response. Standard recommendation to achieve HRC 67/69 is 2150-2175° F.
Tempering: 1000° F minimum recommended. Temper or quadruple tempering required.

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other purposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.