W-1 Steel

Steel name: W-1
Diagram No.: 1782
AISI/SAE designation: W1
UNS designation: T72301
Chemical composition in weight %: 0.70-1.50% C, 0.10-0.40% Si, 0.10-0.40% Mn, max. 0.15% Cr, max. 0.10% Mo, max. 0.10% V, max. 0.15% W
Steel group: Tool steels
Properties: No data
Applications: Blanking dies, cartridge dies, circular cutters, draw dies, drifts, drills, engraving stamps, forming dies, gauges, jeweler dies, knurling tools, paper knives, punches, reamers, striking dies, taps, threading dies, wood knives.
Reference: Not shown in this demo version.

Heat Treatment
Hardening: 1375-1450° F/In water or in a brine solution. Small tools or parts may be heated in molten lead or in a salt bath. Soak time is 10 minutes per inch of thickness. Minimum of 30 minutes.
Tempering: Temper immediately after hardening and quenching. Recommended temperature is 350-550° F.

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other purposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.