VWM2 Steel
Steel name: VWM2
Diagram No.: 1788
ASTM designation: A 600 type M2 (regular C)
EN designation: HS 6-5-2C
AISI/SAE designation: M2
JIS designation: SKH 51
Chemical composition in weight %: 0.90% C, 4.20% Cr, 5.00% Mo, 1.90% V, 6.10% W
Steel group: High speed steels
Properties: No data
Applications: General purpose drills, broaches, reamers, knives, taps, dies or inserts for cold work tooling, where high wear resistance is required, milling cutters, saws.
Reference: Not shown in this demo version.
Heat Treatment
Hardening: Cutting tools: 1180-1220 ºC, cold work dies 1080-1160 ºC. Hardening procedure must involve pre-heating at 400/500 ºC followed by other at 860/880 ºC. For large tools, it is also recommended another pre-heating at 1050 ºC. After pre-heating, hardening at suitable austenitizing temperature may be conducted, followed by quenching down to room temperature. A protective atmosphere is absolutely necessary.
Tempering: 560 ºC. Double tempering treatments, of at least 2h, are required and after each one tools must cool down to room temperature.
Tempering Diagram
Click the image to enlarge the diagram.
Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other purposes. There is no representation that the recipient of this literature will receive updated editions as the become available.