3% Co Steel
Steel name: 3% Co
Diagram No.: 2004
Chemical composition in weight %:
3% Co steel: 0.082% C, 9.16% Cr, 3.27% W, 2.94% Co, 0.19% V, 0.050% Nb, 0.058% N, 0.0047% B
Co-free steel: 0.073% C, 8.93% Cr, 3.23% W, 0.19% V, 0.046% Nb, 0.051% N, 0.0050% B
Steel group: Ferritic steels
Properties: No data
Applications: No data
Reference: Not shown in this demo version.
Heat Treatment
Hardening: See the text bellow.
Tempering: See the diagram.
Diagram note: Two ingots with and without Co were prepared by vacuum induction remelting method. These ingots were hot worked down to 15 mm dia. bars and normalized for 0.5 h at 1373 K followed by air-cooling.
Some coupon were cut from normalized bars and heated for 1.0 h at various temperatures ranging from 773–1113K to know the tempering behavior of these steels. Remaining bars were tempered for 4.0 h at 1043 K to investigate creep properties and microstructures. Moreover, the two steels were aged at 923 K for 1000 h to compare the distribution of precipitates after long-term keeping.
Tempering Diagram
Price: 20.00 US $
Buy Online Tempering Diagram
Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants
Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.