1.2367 Steel

Steel name: 1.2367
Diagram No.: 2020
Mat.No. (Wr.Nr.) designation: 1.2367
Chemical composition in weight %: 0.37% C, 0.42% Si, 0.45% Mn, 4.90% Cr, 2.90% Mo, 0.616% V
Steel group: Hot work tool steels
Properties: No data
Applications: No data
Reference: Not shown in this demo version.

Heat Treatment
Hardening: Specimens were machined into 70x70x25 mm dimensions. All specimens were austenitized 90 min at 1050 °C in vacuum furnace (nitrogen atmosphere). After austenitization, specimens were subjected to two different cooling procedures.
Tempering: See the diagram.
Diagram note: Hardness distribution of specimens tempered at 500 °C and 600 °C. Dashed red line exhibits the hardness distribution of specimens processed at 600 °C before tempering.

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.