WF-XTRA Steel

Steel name: WF-XTRA
Diagram No.: 2044
Chemical composition in weight %: 0.42% C, 0.50% Si, 0.75% Mn, 2.50% Cr, 1.00% Mo, 0.80% Ni, 0.05% V
Steel group: Tool steels
Properties: No data
Applications: Hammer dies, press dies, insert dies, punches, extrusion dies, headers, gripper dies and gripper inserts, casting, dies.
Reference: Not shown in this demo version.

Heat Treatment
Hardening: Increasing the hardness requires heating to an austenitizing temperature (1550-1600 F/840-870 C) followed by a quenching operation. (Some oxidation/ decarburization will occur on the block surface unless heating is performed in a vacuum or protective atmosphere furnace.) Quenching is a high stress operation introducing a risk of cracking, particularly for a machined block with contours, sharp edges, drilled holes or thin-web features. For such product, employing a quenchant with a lower quenchseverity rating will lower the risk of cracking.
Tempering: See the diagram.
Diagram note: No data

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.