1.2379 Steel

Steel name: 1.2379
Diagram No.: 2149
DIN designation: X155CrVMo121
Mat.No. (Wr.Nr.) designation: 1.2379
AISI/SAE designation: D2
UNI designation: (X155CrVMo121KU)
AFNOR designation: (Z160CDV12)
GB designation: BD2
Chemical composition in weight %: 1.50-1.60% C, 0.10-0.40% Si, 0.15-0.45% Mn, 11.00-12.00% Cr, 0.60-0.80% Mo, 0.90-1.10% V
Steel group: Cold work tool steels
Applications: No data
Note: Ac1=820 C, Ms=190 C
Reference: Not shown in this demo version.

Heat Treatment
Hardening: 1010-1040 °C or at 1080-1100 °C; cooling in air or in oil if large parts.
Tempering: In the temperature range 150-300 °C with minimum holding time of 3 h. For parts hardened at 1080-1100 °C, a first tempering will be carried out at 500-550 °C in order to exploit secondary hardness, followed by a second tempering at 180/300 °C.
Diagram note: No data

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.