Idun Steel

Steel name: Idun
Diagram No.: 2194
Chemical composition in weight %: 0.21% C, 0.90% Si, 0.45% Mn, 13.50% Cr, 0.20% Mo, 0.60% Ni, 0.25% V, +N
Steel group: Stainless tool steels
Properties: No data
Applications: No data
Reference: Not shown in this demo version.

Heat Treatment
Hardening: Preheating temperature: 500–600°C (930– 1110°F). Austenitizing temperature: 980–1000°C (1800– 1830°F) but usually 980°C (1800°F). Quenching media: Vacuum with sufficient positive pressure. High speed gas/circulating atmosphere.
Tempering: Choose the tempering temperature according to the hardness required by reference to the tempering graph. Temper minimum twice with intermediate cooling to room temperature. Lowest tempering temperature 250°C (480°F). Holding time at temperature minimum 2 hours.
Diagram note: Bellow tempering curve is obtained after heat treatment of samples with a size of 15 x 15 x 40 mm, cooling in forced air. Lower hardness can be expected after heat treatment of tools, components and dies due to factors like the actual size of the part and heat treatment parameters.

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.