416R Steel

Steel name: 416R
Diagram No.: 2198
AISI/SAE designation: 416R
Chemical composition in weight %: 0.12% C, 0.40% Si, 0.40% Mn, 0.03% P, 0.13% S, 12.50% Cr, 0.40% Mo
Steel group: Chromium stainless steels
Properties: 416R is a hardenable chromium stainless steel particularly suited for use in high quality precision rifle barrels. This grade has good machinability and, because of closely controlled chemistry and processing techniques, may be machined and lapped to a high finish, which is important for bore accuracy.
Applications: No data
Reference: Not shown in this demo version.

Heat Treatment
Hardening: 416R can be hardened by air cooling or oil quenching from 1750 to 1850°F (954 to 1010°C). When air hardening small or thin sections, a temperature in the upper part of this range should be used. Tempering should be at the proper temperature to give the desired properties as shown below.
Tempering: See the diagram.
Diagram note: No data

Diagram Tempering Temperature - Mechanical Properties

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.