1.2210 Steel

Steel name: 1.2210
Diagram No.: 2218
Mat.No. (Wr.Nr.) designation: 1.2210
DIN designation: 115CrV3
AISI/SAE designation: L2
Chemical composition in weight %: 1.18% C, 0.25% Si, 0.30% Mn, 0.70% Cr, 0.10% V
Steel group: Cold work tool steels
Properties: Chrome-Vanadium alloyed cold-work steel with high resistance; also known as silver steel.
Applications: Small turned parts, core pins, punches and engraving tools.
Reference: Not shown in this demo version.

Heat Treatment
Hardening: 780 to 840 °C, 15 to 30 minutes keeping curing temperature quenching in water/oil, obtainable hardness: 64-66 HRC.
Tempering: Slow heating to tempering temperature immediately after hardening; minimum time in furnace: 1 hour per 20 mm part thickness; min. 2 hours/cooling in air.
Diagram note: No data

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.