1.2764 Steel

Steel name: ECN4M
Diagram No.: 2408
Mat.No. (Wr.Nr.) designation: 1.2764
DIN designation: X19NiCrMo4
Chemical composition in weight %: 0.19% C, 1.30% Cr, 0.20% Mo, 4.10% Ni
Steel group: Case hardening steels
Properties: Case hardening steel, when hardened high core strength, good polishability in hardened condition.
Applications: Press tools, highly stressed plastic moulds, profiling rolls.
Reference: Not shown in this demo version.

Heat Treatment
Carburizing: 860 - 890°C
Hardening: 780 - 810°C, oil or hot bath 180 - 220°C.
Hardening: 800 - 830°C, air.
Tempering: See the diagram.
Diagram note: No data

Tempering Diagram (For Carburized Surface)

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.