Q10 Steel

Steel name: Q10
Diagram No.: 2484
Chemical composition in weight %: 0.36% C, 0.25% Si, 0.40% Mn, 5.20% Cr, 1.90% Mo, 0.55% V
Steel group: Hot work tool steels
Properties: Q10 is a Cr-Mo-V-alloyed premium steel. In addition to high toughness, it offers very good high-temperature strength properties and a good thermal shock resistance.
Applications: Extrusion presses with very long lifetime with heavy duty inner linings and press stems, dies and die holder. Die forging: dies subject to high impact stress, dies with complex geometry, which are exposed to both high abrasive wear and simultaneous risk of cracking. Drawing mandrels. Tools for the production of seamless gas cylinders.
Reference: Not shown in this demo version.

Heat Treatment
Hardening: 1010 - 1020 °C. Air, warm bath of approx. 540 °C, Oil/polymer; Interrupt oil or polymer cooling at 230 - 280 °C or vacuum hardening.
Tempering: 540 - 680 °C.
Diagram note: No data

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.