UH1 Steel

Steel name: UH1
Diagram No.: 2487
Chemical composition in weight %: 0.46% C, 0.45% Si, 0.50% Mn, 6.70% Cr, 1.50% Mo, 0.80% V
Steel group: Hot work tool steels
Properties: UH1 is a Cr-Mo-V-alloyed hot-work tool steel which is characterized by an outstanding wear resistance. In addition, the steel offers good high-temperature strength. The exclusive production using the ESR process confers the steel UH1 a good toughness even at high hardness level.
Applications: The newly developed steel UH1 with his excellent wear resistance fulfills the current demand of the hot stamping market. Further possible applications: Highly stressed extruder cylinders in plastics processing. Cutting and punching tools.
Reference: Not shown in this demo version.

Heat Treatment
Hardening: 1040 - 1070 °C. Air, warm bath of approx. 540 °C, Oil/polymer; Interrupt oil or polymer cooling at 250 - 300 °C or vacuum hardening.
Tempering: 500 - 700 °C.
Diagram note: No data

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.