Rigor Steel

Steel name: Rigor
Diagram No.: 2746
Mat.No. (Wr.Nr.) designation: 1.2363.
EN designation: X100CrMoV5
AISI/SAE designation: A2
Chemical composition in weight %: 1.00% C, 0.30% Si, 0.60% Mn, 5.30% Cr, 1.10% Mo, 0.20% V
Steel group: Tool steels
Properties: No data
Applications: Uddeholm Rigor takes a place in the Uddeholm tool steel range between Uddeholm Arne and Uddeholm Sverker 21, offering an excellent combination of good wear resistance and toughness. It may be regarded, therefore, as a “universal” cold work steel. For cutting operations the good toughness of Uddeholm Rigor gives excellent resistance to chipping of the cutting edge. In many cases tools made from this steel have given better tooling economy than high-carbon, highchromium steel of the BD3/W.-Nr. 2080 type. Uddeholm Rigor has much better machining and grinding properties.
Reference: Not shown in this demo version.

Heat Treatment
Hardening: Preheating temperature: 650–750°C (1200– 1300°F). Austenitizing temperature: 925–970°C (1690– 1780°F) but usually 940–960°C (1720– 1760°F). Quenching media: Martempering bath or fluidized bed at 180–220°C (360–430°F) or 450–550°C (840–1020°F) then cool in air. Circulating air or atmosphere. Vacuum furnace with overpressure of gas at cooling. Oil (only for small and uncomplicated tools).
Tempering: Choose the tempering temperature according to the hardness required by reference to the tempering graph. Temper twice with intermediate cooling to room temperature. Lowest tempering temperature 180°C (360°F). Holding time at temperature minimum 2 hours.
Diagram note: The tempering graphs are valid for small samples. The hardness received is also dependent on the tool size.

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.