Unimax Steel

Steel name: Unimax
Diagram No.: 2766
Chemical composition in weight %: 0.50% C, 0.20% Si, 0.50% Mn, 5.00% Cr, 2.30% Mo, 0.50% V
Steel group: Plastic mould steels
Properties: Uddeholm Unimax is a ESR remelted chromium-molybdenum-vanadium alloyed tool steel.
Applications: Uddeholm Unimax is suitable for long run production moulds, moulds for reinforced plastics and compression moulding. Uddeholm Unimax is a problem solver in severe cold work tooling applications such as heavy duty blanking, cold forging and thread rolling, where high chipping resistance is required. Engineering and hot work applications requiring high hardness and toughness are also an option.
Reference: Not shown in this demo version.

Heat Treatment
Hardening: Preheating temperature: 600–650°C (1110– 1200°F) and 850–900°C (1560–1650°F). Austenitizing temperature: 1000–1025°C (1830–1875°F), normally 1025°C (1875°F). Holding time: 30 minutes.
Quenching media: High speed gas/circulating atmosphere. Vacuum furnace (high speed gas with sufficient overpressure). Martempering bath, salt bath or fluidized bed at 300–550°C (570–1020°F).
Tempering: Choose the tempering temperature according to the hardness required by reference to the tempering graph below.
Diagram note: The tempering curves are obtained after heat treatment of samples with a size of 15 x 15 x 40 mm, cooling in forced air. Lower hardness can be expected after heat treatment of tools and dies due to factors like actual tool size and heat treatment parameters.

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.