1.2343 Steel

Steel name: 1.2343
Diagram No.: 2783
Mat.No. (Wr.Nr.) designation: ~1.2343
AISI/SAE designation: H11 mod.
Chemical composition in weight %: 0.36% C, 0.20% Si, 0.30% Mn, 5.00% Cr, 1.35% Mo, 0.45% V
Steel group: Hot work tool steels
Properties: No data
Applications: This steel is primarily designed for die casting of light metals and alloys. It is often used for highly stressed hot-work structural parts where superior toughness is required (up to average Charpy V-notch value of 29.8 Joule at 44-46 HRC according to NADCA#207).
Reference: Not shown in this demo version.

Heat Treatment
Hardening: 980 - 1000 °C. Fast cooling is recommended in pressurized N2. For large dimension hot-work tooling see NADCA#207 or GM DC-9999-1Rev.18 specification.
Tempering: 520 - 530 °C, cool in air or in the furnace to room temperature between tempering cycles.
Diagram note: No data

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.