V4E Steel

Steel name: V4E
Diagram No.: 2841
Chemical composition in weight %: 1.40% C, 0.40% Si, 0.40% Mn, 4.70% Cr, 3.50% Mo, 3.70% V
Steel group: PM cold work tool steels
Properties: No data
Applications: No data
Reference: Not shown in this demo version.

Heat Treatment
Hardening: Pre-heating temperature: First pre-heating at 600–650°C (1110–1200°F) and second at 850–900°C (1560–1650°F).
Austenitizing temperature: 940–1180°C (1725–2160°F), normally 1020°C (1870°F).
• For large sections, i.e. >70 mm (2.75”) use 1060°C (1940°F).
• For the very best wear resistance use 1100–1180°C (2010–2160°F).
Soaking time: 30 min. for hardening temper.atures up to 1100°C (2010°F), 15 min. for temperatures higher than 1100°C (2010°F).
Vacuum (high speed gas at sufficient over.pressure, minimum 2 bar). Martempering bath or fluidized bed at 200–550°C (390–1020°F). Forced air/gas
Tempering: Choose the tempering temperature according to the hardness required by reference to the tempering graphs. Temper at least twice with intermediate cooling to room temperature. For highest dimensional stability and ductil.ity, a minimum temperature of 540°C (1000°F) and three tempers is strongly recommended. Tempering at a lower temperature than 540°C (1000°F) may increase the hardness and compressive strength to some extent but also impair cracking resistance and dimensional stability. However, if lowering the tempering temperature, do not temper below 520°C (970°F).
Diagram note: Vanadis 4 Extra SuperClean steel.

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other puposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.