420 HC Steel

Steel name: 420 HC
Diagram No.: 776
Chemical composition in weight %: 0.46% C, 0.40% Si, 0.40% Mn, 13.00% Cr, 0.30% V
Steel group: High-carbon martensitic stainless steels
Properties: No data
Applications: 420 HC should be considered for applications such as specialty knives, industrial knives, cutlery, rolls, plastic extrusion tooling, scissors, surgical knives, bearings, and other applications which require a combination of corrosion resistance and wear resistance.
Reference: Not shown in this demo version.

Heat Treatment
Hardening: 982-1025oC/air, gas, oil
Tempering: See the diagram
Diagram note: Air cooled from 1010oC and double tempered.

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other purposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.