Ovako 803Q Steel

Steel name: Ovako 803Q
Diagram No.: 87
DIN: 100Cr6
SAE: 52100
AFNOR NF: 100Cr6
JIS: SUJ2
Chemical composition in weight %: 0.93% C, 0.28% Mn, 0.28% Si, 0.009% P, 0.001% S, 1.47% Cr, 0.02% Mo, 0.10% Ni, 0.10 Cu, 12 ppm Ti, 3.9 ppm O.
Properties: Structural steel, high clean steel.
Reference: Not shown in this demo version.

Heat Treatment
Martensitic hardening: 830-870°C, 10-60 min, oil quench (+ tempering within 2 hrs)
Bainitic hardening: 850-875°C, 10-60 min, Salt bath 220-250°C, 3-7 hrs
Tempering: 160-500oC
Diagram note: The diagram data: Austenized at 840°C, oil quenched and tempered 1h.

Tempering Diagram

Price: 20.00 US $
Buy Online Tempering Diagram

Other Steel Data links
Carbides in Steel
CCT and TTT Diagrams of Steels
CCT and TTT Diagram Calculating Service
Hardenability Diagrams of Steels
Hardenability Calculating Service
Macro Defects in Steel
Metal Etchants
Non-Metallic Inclusions in Steel
Semiconductor Etchants

Disclaimer: The material data is a central depository of information based on global actual tests and calculated software data that is available to the public for a fee. The information and data presented herein are typical or average values and are not a guarantee of maximum or minimum values. Applications specifically suggested for material described herein are made solely for the purpose of illustration to enable the reader to make his own evaluation and are not intended as warranties, either express or implied, of fitness for these or other purposes. There is no representation that the recipient of this literature will receive updated editions as the become available.

Copyright © 2023 by Steel Data. All Rights Reserved.