Hardness Conversion Chart

 Brinell Hardness  Vickers Hardness  Rockwell Hardness  Tensile Strength
 100 HB   105 HV   - HRC   335 N/mm2
 101 HB   106 HV   - HRC   338 N/mm2
 102 HB  107 HV  - HRC  341 N/mm2
 103 HB  108 HV  - HRC  344 N/mm2
 104 HB  109 HV  - HRC  347 N/mm2
 105 HB  110 HV  - HRC  350 N/mm2
 106 HB  111 HV  - HRC  355 N/mm2
 107 HB  112 HV  - HRC  360 N/mm2
 108 HB  113 HV  - HRC  365 N/mm2
 109 HB  114 HV  - HRC  370 N/mm2
 110 HB  115 HV  - HRC  373 N/mmø
 111 HB  116 HV  - HRC  376 N/mm2
 112 HB  117 HV  - HRC  379 N/mm2
 113 HB  118 HV  - HRC  382 N/mm2
 114 HB  119 HV  - HRC  385 N/mm2
 115 HB  120 HV  - HRC  388 N/mm2
 116 HB  121 HV  - HRC  391 N/mm2
 117 HB  122 HV  - HRC  394 N/mm2
 118 HB  123 HV  - HRC  397 N/mm2
 119 HB  125 HV  - HRC  400 N/mm2
 120 HB  126 HV  - HRC  403 N/mm2
 121 HB  127 HV  - HRC  406 N/mm2
 122 HB  128 HV  - HRC  409 N/mm2
 123 HB  129 HV  - HRC  412 N/mm2
 124 HB  130 HV  - HRC  415 N/mm2
 125 HB  131 HV  - HRC  418 N/mm2
 126 HB  132 HV  - HRC  422 N/mm2
 127 HB  133 HV  - HRC  426 N/mm2
 128 HB  135 HV  - HRC  430 N/mm2
 129 HB  136 HV  - HRC  434 N/mm2
 130 HB  137 HV  - HRC  438 N/mm2
 131 HB  138 HV  - HRC  442 N/mm2
 132 HB  139 HV  - HRC  446 N/mm2
 133 HB  140 HV  - HRC  450 N/mm2
 134 HB  141 HV  - HRC  453 N/mm2
 135 HB  142 HV  - HRC  456 N/mm2
 136 HB  143 HV  - HRC  459 N/mm2
 137 HB  144 HV  - HRC  462 N/mm2
 138 HB  145 HV  - HRC  465 N/mm2
 139 HB  146 HV  - HRC  468 N/mm2
 140 HB  147 HV  - HRC  471 N/mm2
 141 HB  148 HV  - HRC  474 N/mm2
 142 HB  149 HV  - HRC  477 N/mm2
 143 HB  150 HV  - HRC  480 N/mm2
 144 HB  151 HV  - HRC  484 N/mm2
 145 HB  152 HV  - HRC  488 N/mm2
 146 HB  153 HV  - HRC  492 N/mm2
 147 HB  155 HV  - HRC  495 N/mm2
 148 HB  156 HV  - HRC  498 N/mm2
 149 HB  157 HV  - HRC  501 N/mm2
 150 HB  158 HV  - HRC  504 N/mm2
 151 HB  159 HV  - HRC  507 N/mm2
 152 HB  160 HV  - HRC  510 N/mm2
 153 HB  161 HV  - HRC  515 N/mm2
 154 HB  162 HV  - HRC  520 N/mm2
 155 HB  163 HV  - HRC  525 N/mm2
 156 HB  164 HV  - HRC  530 N/mm2
 157 HB  165 HV  - HRC  532 N/mm2
 158 HB  166 HV  - HRC  534 N/mm2
 159 HB  167 HV  - HRC  537 N/mm2
 160 HB  168 HV  - HRC  539 N/mm2
 161 HB  116 HV  - HRC  542 N/mm2
 162 HB  170 HV  - HRC  545 N/mm2
 163 HB  171 HV  - HRC  549 N/mm2
 164 HB  172 HV  - HRC  553 N/mm2
 165 HB  173 HV  - HRC  557 N/mm2
 166 HB  174 HV  - HRC  560 N/mm2
 167 HB  175 HV  - HRC  563 N/mm2
 168 HB  176 HV  - HRC  566 N/mm2
 169 HB  177 HV  - HRC  569 N/mm2
 170 HB  179 HV  - HRC  572 N/mm2
 171 HB  180 HV  - HRC  575 N/mm2
 172 HB  181 HV  - HRC  579 N/mm2
 173 HB  182 HV  - HRC  583 N/mm2
 174 HB  183 HV  - HRC  587 N/mm2
 175 HB  184 HV  - HRC  591 N/mm2
 176 HB  185 HV  - HRC  595 N/mm2
 177 HB  186 HV  - HRC  598 N/mm2
 178 HB  187 HV  - HRC  601 N/mm2
 179 HB  188 HV  - HRC  604 N/mm2
 180 HB  189 HV  - HRC  607 N/mm2
 181 HB  190 HV  - HRC  610 N/mm2
 182 HB  191 HV  - HRC  613 N/mm2
 183 HB  192 HV  - HRC  617 N/mm2
 184 HB  193 HV  - HRC  621 N/mm2
 185 HB  194 HV  - HRC  625 N/mm2
 186 HB  195 HV  - HRC  628 N/mm2
 187 HB  196 HV  - HRC  631 N/mm2
 188 HB  197 HV  - HRC  634 N/mm2
 189 HB  199 HV  - HRC  637 N/mm2
 190 HB  200 HV  - HRC  640 N/mm2
 191 HB  201 HV  - HRC  644 N/mm2
 192 HB  202 HV  - HRC  648 N/mm2
 193 HB  203 HV  - HRC  652 N/mm2
 194 HB  204 HV  - HRC  656 N/mm2
 195 HB  205 HV  - HRC  660 N/mm2
 196 HB  206 HV  - HRC  663 N/mm2
 197 HB  207 HV  - HRC  667 N/mm2
 198 HB  208 HV  - HRC  671 N/mm2
 199 HB  209 HV  - HRC  675 N/mm2
 200 HB  210 HV  - HRC  678 N/mm2
 201 HB  211 HV  - HRC  681 N/mm2
 202 HB  212 HV  - HRC  684 N/mm2
 203 HB  213 HV  - HRC  687 N/mm2
 204 HB  214 HV  - HRC  690 N/mm2
 205 HB  215 HV  - HRC  693 N/mm2
 206 HB  216 HV  - HRC  696 N/mm2
 207 HB  217 HV  - HRC  699 N/mm2
 208 HB  218 HV  - HRC  702 N/mm2
 209 HB  220 HV  - HRC  705 N/mm2
 210 HB  221 HV  - HRC  708 N/mm2
 211 HB  222 HV  - HRC  711 N/mm2
 212 HB  223 HV  - HRC  714 N/mm2
 213 HB  224 HV  - HRC  717 N/mm2
 214 HB  225 HV  - HRC  720 N/mm2
 215 HB  226 HV  - HRC  724 N/mm2
 216 HB  227 HV  - HRC  728 N/mm2
 217 HB  228 HV  - HRC  732 N/mm2
 218 HB  229 HV  - HRC  736 N/mm2
 219 HB  230 HV  - HRC  740 N/mm2
 220 HB  231 HV  - HRC  744 N/mm2
 221 HB  232 HV  - HRC  748 N/mm2
 222 HB  233 HV  - HRC  752 N/mm2
 223 HB  234 HV  - HRC  755 N/mm2
 224 HB  235 HV  - HRC  758 N/mm2
 225 HB  236 HV  - HRC  761 N/mm2
 226 HB  237 HV  - HRC  763 N/mm2
 227 HB  238 HV  - HRC  767 N/mm2
 228 HB  240 HV  20.3 HRC  770 N/mm2
 229 HB  241 HV  20.5 HRC  773 N/mm2
 230 HB  242 HV  20.7 HRC  776 N/mm2
 231 HB  243 HV  20.9 HRC  779 N/mm2
 232 HB  244 HV  21.1 HRC  782 N/mm2
 233 HB  245 HV  21.3 HRC  785 N/mm2
 234 HB  246 HV  21.5 HRC  788 N/mm2
 235 HB  247 HV  21.7 HRC  791 N/mm2
 236 HB  248 HV  21.9 HRC  793 N/mm2
 237 HB  249 HV  22.0 HRC  797 N/mm2
 238 HB  250 HV  22.2 HRC  800 N/mm2
 239 HB  251 HV  22.5 HRC  805 N/mm2
 240 HB  252 HV  22.7 HRC  810 N/mm2
 241 HB  253 HV  22.9 HRC  815 N/mm2
 242 HB  254 HV  23.1 HRC  820 N/mm2
 243 HB  255 HV  23.3 HRC  821 N/mm2
 244 HB  256 HV  23.5 HRC  824 N/mm2
 245 HB  257 HV  23.7 HRC  827 N/mm2
 246 HB  258 HV  23.9 HRC  831 N/mm2
 246 HB  258 HV  23.9 HRC  831 N/mm2
 247 HB  260 HV  24.0 HRC  835 N/mm2
 248 HB  261 HV  24.2 HRC  838 N/mm2
 249 HB  262 HV  24.3 HRC  841 N/mm2
 250 HB  263 HV  24.5 HRC  844 N/mm2
 251 HB  264 HV  24.7 HRC  847 N/mm2
 252 HB  265 HV  24.8 HRC  850 N/mm2
 253 HB  266 HV  25.0 HRC  853 N/mm2
 254 HB  267 HV  25.1 HRC  856 N/mm2
 255 HB  268 HV  25.3 HRC  859 N/mm2
 256 HB  269 HV  25.5 HRC  862 N/mm2
 257 HB  270 HV  25.6 HRC  865 N/mm2
 258 HB  271 HV  25.8 HRC  869 N/mm2
 259 HB  272 HV  26.0 HRC  873 N/mm2
 260 HB  273 HV  26.2 HRC  877 N/mm2
 261 HB  274 HV  26.4 HRC  880 N/mm2
 262 HB  275 HV  26.6 HRC  884 N/mm2
 263 HB  276 HV  26.7 HRC  888 N/mm2
 264 HB  277 HV  26.8 HRC  892 N/mm2
 265 HB  278 HV  26.9 HRC  896 N/mm2
 266 HB  280 HV  27.1 HRC  900 N/mm2
 267 HB  281 HV  27.3 HRC  903 N/mm2
 268 HB  282 HV  27.4 HRC  906 N/mm2
 269 HB  283 HV  27.5 HRC  909 N/mm2
 270 HB  284 HV  27.6 HRC  912 N/mm2
 271 HB  285 HV  27.8 HRC  915 N/mm2
 272 HB  286 HV  28.0 HRC  918 N/mm2
 273 HB  287 HV  28.1 HRC  921 N/mm2
 274 HB  288 HV  28.3 HRC  924 N/mm2
 275 HB  289 HV  28.4 HRC  927 N/mm2
 276 HB  290 HV  28.5 HRC  930 N/mm2
 277 HB  291 HV  28.7 HRC  935 N/mm2
 278 HB  292 HV  28.9 HRC  940 N/mm2
 279 HB  293 HV  29.0 HRC  945 N/mm2
 280 HB  294 HV  29.2 HRC  950 N/mm2
 281 HB  295 HV  29.3 HRC  953 N/mm2
 282 HB  296 HV  29.4 HRC  956 N/mm2
 283 HB  297 HV  29.5 HRC  959 N/mm2
 284 HB  298 HV  29.6 HRC  962 N/mm2
 285 HB  300 HV  29.8 HRC  965 N/mm2
 286 HB  301 HV  30.0 HRC  968 N/mm2
 287 HB  302 HV  30.2 HRC  971 N/mm2
 288 HB  303 HV  30.3 HRC  974 N/mm2
 289 HB  304 HV  30.4 HRC  977 N/mm2
 290 HB  305 HV  30.5 HRC  980 N/mm2
 291 HB  306 HV  30.6 HRC  983 N/mm2
 292 HB  307 HV  30.7 HRC  986 N/mm2
 293 HB  308 HV  30.8 HRC  989 N/mm2
 294 HB  309 HV  30.9 HRC  992 N/mm2
 295 HB  310 HV  31.0 HRC  995 N/mm2
 296 HB  311 HV  31.1 HRC  999 N/mm2
 297 HB  312 HV  31.2 HRC  1004 N/mm2
 298 HB  313 HV  31.3 HRC  1008 N/mm2
 299 HB  314 HV  31.4 HRC  1012 N/mm2
 300 HB  315 HV  31.6 HRC  1015 N/mm2
 301 HB  316 HV  31.8 HRC  1019 N/mm2
 302 HB  317 HV  31.9 HRC  1013 N/mm2
 303 HB  318 HV  32.0 HRC  1027 N/mm2
 304 HB  320 HV  32.2 HRC  1030 N/mm2
 305 HB  321 HV  32.3 HRC  1033 N/mm2
 306 HB  322 HV  32.4 HRC  1036 N/mm2
 307 HB  323 HV  32.5 HRC  1039 N/mm2
 308 HB  324 HV  32.6 HRC  1042 N/mm2
 309 HB  325 HV  32.7 HRC  1045 N/mm2
 310 HB  326 HV  32.8 HRC  1048 N/mm2
 311 HB  327 HV  32.9 HRC  1051 N/mm2
 312 HB  328 HV  33.0 HRC  1054 N/mm2
 312 HB  328 HV  33.0 HRC  1054 N/mm2
 313 HB  329 HV  33.1 HRC  1057 N/mm2
 314 HB  330 HV  33.3 HRC  1060 N/mm2
 315 HB  331 HV  33.4 HRC  1063 N/mm2
 316 HB  332 HV  33.6 HRC  1067 N/mm2
 317 HB  333 HV  33.7 HRC  1071 N/mm2
 318 HB  334 HV  33.8 HRC  1075 N/mm2
 319 HB  335 HV  33.9 HRC  1079 N/mm2
 320 HB  336 HV  34.0 HRC  1083 N/mm2
 321 HB  337 HV  34.1 HRC  1087 N/mm2
 322 HB  338 HV  34.2 HRC  1091 N/mm2
 323 HB  339 HV  34.4 HRC  1095 N/mm2
 324 HB  340 HV  34.5 HRC  1098 N/mm2
 325 HB  341 HV  34.6 HRC  1101 N/mm2
 326 HB  342 HV  34.7 HRC  1104 N/mm2
 327 HB  343 HV  34.9 HRC  1107 N/mm2
 328 HB  344 HV  35.0 HRC  1110 N/mm2
 329 HB  345 HV  35.1 HRC  1113 N/mm2
 330 HB  346 HV  35.2 HRC  1116 N/mm2
 331 HB  347 HV  35.3 HRC  1119 N/mm2
 332 HB  348 HV  35.4 HRC  1122 N/mm2
 333 HB  350 HV  35.5 HRC  1125 N/mm2
 334 HB  351 HV  35.6 HRC  1128 N/mm2
 335 HB  352 HV  35.7 HRC  1131 N/mm2
 336 HB  353 HV  35.9 HRC  1135 N/mm2
 337 HB  354 HV  36.0 HRC  1138 N/mm2
 338 HB  355 HV  36.1 HRC  1141 N/mm2
 339 HB  356 HV  36.2 HRC  1145 N/mm2
 340 HB  357 HV  36.3 HRC  1149 N/mm2
 341 HB  358 HV  36.4 HRC  1152 N/mm2
 342 HB  359 HV  36.6 HRC  1155 N/mm2
 343 HB  360 HV  36.7 HRC  1158 N/mm2
 344 HB  361 HV  36.9 HRC  1162 N/mm2
 345 HB  362 HV  37.0 HRC  1165 N/mm2
 346 HB  363 HV  37.1 HRC  1169 N/mm2
 347 HB  364 HV  37.2 HRC  1172 N/mm2
 348 HB  365 HV  37.3 HRC  1176 N/mm2
 349 HB  366 HV  37.4 HRC  1179 N/mm2
 350 HB  367 HV  37.5 HRC  1183 N/mm2
 351 HB  368 HV  37.6 HRC  1187 N/mm2
 352 HB  370 HV  37.7 HRC  1190 N/mm2
 353 HB  371 HV  37.8 HRC  1194 N/mm2
 354 HB  372 HV  38.0 HRC  1197 N/mm2
 355 HB  373 HV  38.1 HRC  1201 N/mm2
 356 HB  374 HV  38.2 HRC  1205 N/mm2
 357 HB  375 HV  38.4 HRC  1208 N/mm2
 358 HB  376 HV  38.5 HRC  1211 N/mm2
 359 HB  377 HV  38.6 HRC  1214 N/mm2
 360 HB  378 HV  38.7 HRC  1217 N/mm2
 361 HB  380 HV  38.8 HRC  1220 N/mm2
 362 HB  381 HV  38.9 HRC  1224 N/mm2
 363 HB  382 HV  39.0 HRC  1227 N/mm2
 364 HB  383 HV  39.1 HRC  1231 N/mm2
 365 HB  384 HV  39.2 HRC  1234 N/mm2
 366 HB  385 HV  39.3 HRC  1237 N/mm2
 367 HB  386 HV  39.4 HRC  1241 N/mm2
 368 HB  387 HV  39.5 HRC  1244 N/mm2
 369 HB  388 HV  39.6 HRC  1247 N/mm2
 370 HB  389 HV  39.7 HRC  1251 N/mm2
 370 HB  389 HV  39.7 HRC  1251 N/mm2
 371 HB  390 HV  39.8 HRC  1255 N/mm2
 372 HB  391 HV  39.9 HRC  1259 N/mm2
 373 HB  392 HV  40.0 HRC  1263 N/mm2
 374 HB  393 HV  40.1 HRC  1267 N/mm2
 375 HB  394 HV  40.2 HRC  1271 N/mm2
 376 HB  395 HV  40.3 HRC  1275 N/mm2
 377 HB  396 HV  40.4 HRC  1278 N/mm2
 378 HB  397 HV  40.5 HRC  1282 N/mm2
 379 HB  398 HV  40.6 HRC  1286 N/mm2
 380 HB  400 HV  40.8 HRC  1290 N/mm2
 381 HB  401 HV  40.9 HRC  1293 N/mm2
 382 HB  402 HV  41.0 HRC  1296 N/mm2
 383 HB  403 HV  41.1 HRC  1299 N/mm2
 384 HB  404 HV  41.2 HRC  1302 N/mm2
 385 HB  405 HV  41.3 HRC  1305 N/mm2
 386 HB  406 HV  41.4 HRC  1308 N/mm2
 387 HB  407 HV  41.5 HRC  1311 N/mm2
 388 HB  408 HV  41.6 HRC  1314 N/mm2
 389 HB  409 HV  41.7 HRC  1317 N/mm2
 390 HB  410 HV  41.8 HRC  1320 N/mm2
 391 HB  411 HV  41.9 HRC  1324 N/mm2
 392 HB  412 HV  42.0 HRC  1328 N/mm2
 393 HB  413 HV  42.1 HRC  1332 N/mm2
 394 HB  414 HV  42.2 HRC  1335 N/mm2
 395 HB  415 HV  42.3 HRC  1338 N/mm2
 396 HB  416 HV  42.4 HRC  1342 N/mm2
 397 HB  417 HV  42.5 HRC  1345 N/mm2
 398 HB  418 HV  42.6 HRC  1347 N/mm2
 399 HB  420 HV  42.7 HRC  1350 N/mm2
 400 HB  421 HV  42.8 HRC  1353 N/mm2
 401 HB  422 HV  42.9 HRC  1357 N/mm2
 402 HB  423 HV  43.0 HRC  1360 N/mm2
 403 HB  424 HV  43.1 HRC  1364 N/mm2
 404 HB  425 HV  43.2 HRC  1367 N/mm2
 405 HB  426 HV  43.3 HRC  1371 N/mm2
 406 HB  427 HV  43.4 HRC  1373 N/mm2
 407 HB  428 HV  43.5 HRC  1377 N/mm2
 408 HB  429 HV  43.5 HRC  1381 N/mm2
 409 HB  430 HV  43.6 HRC  1385 N/mm2
 410 HB  431 HV  43.7 HRC  1389 N/mm2
 411 HB  432 HV  43.8 HRC  1393 N/mm2
 412 HB  433 HV  43.9 HRC  1397 N/mm2
 413 HB  434 HV  44.0 HRC  1400 N/mm2
 414 HB  435 HV  44.1 HRC  1404 N/mm2
 415 HB  436 HV  44.2 HRC  1407 N/mm2
 416 HB  437 HV  44.3 HRC  1411 N/mm2
 417 HB  438 HV  44.4 HRC  1415 N/mm2
 418 HB  440 HV  44.5 HRC  1420 N/mm2
 419 HB  441 HV  44.6 HRC  1424 N/mm2
 420 HB  442 HV  44.7 HRC  1427 N/mm2
 421 HB  443 HV  44.8 HRC  1431 N/mm2
 422 HB  444 HV  44.9 HRC  1434 N/mm2
 423 HB  445 HV  45.0 HRC  1437 N/mm2
 424 HB  446 HV  45.1 HRC  1441 N/mm2
 425 HB  447 HV  45.1 HRC  1445 N/mm2
 426 HB  448 HV  45.2 HRC  1448 N/mm2
 427 HB  449 HV  45.2 HRC  1452 N/mm2
 428 HB  450 HV  45.3 HRC  1455 N/mm2
 429 HB  451 HV  45.3 HRC  1458 N/mm2
 430 HB  452 HV  45.4 HRC  1461 N/mm2
 431 HB  453 HV  45.5 HRC  1464 N/mm2
 432 HB  454 HV  45.6 HRC  1468 N/mm2
 433 HB  455 HV  45.7 HRC  1471 N/mm2
 434 HB  456 HV  45.8 HRC  1474 N/mm2
 435 HB  457 HV  45.9 HRC  1478 N/mm2
 436 HB  458 HV  46.0 HRC  1482 N/mm2
 437 HB  460 HV  46.1 HRC  1485 N/mm2
 438 HB  461 HV  46.2 HRC  1488 N/mm2
 439 HB  462 HV  46.3 HRC  1491 N/mm2
 440 HB  463 HV  46.4 HRC  1494 N/mm2
 441 HB  464 HV  46.5 HRC  1498 N/mm2
 442 HB  465 HV  46.6 HRC  1502 N/mm2
 443 HB  466 HV  46.6 HRC  1506 N/mm2
 444 HB  467 HV  46.7 HRC  1509 N/mm2
 445 HB  468 HV  46.7 HRC  1512 N/mm2
 446 HB  469 HV  46.8 HRC  1516 N/mm2
 447 HB  470 HV  46.9 HRC  1520 N/mm2
 448 HB  471 HV  47.0 HRC  1524 N/mm2
 449 HB  472 HV  47.1 HRC  1528 N/mm2
 450 HB  473 HV  47.1 HRC  1532 N/mm2
 451 HB  474 HV  47.2 HRC  1534 N/mm2
 452 HB  475 HV  47.3 HRC  1538 N/mm2
 453 HB  476 HV  47.4 HRC  1542 N/mm2
 454 HB  477 HV  47.5 HRC  1546 N/mm2
 455 HB  478 HV  47.6 HRC  1550 N/mm2
 456 HB  480 HV  47.7 HRC  1555 N/mm2
 457 HB  481 HV  47.7 HRC  1559 N/mm2
 458 HB  482 HV  47.8 HRC  1563 N/mm2
 459 HB  483 HV  47.9 HRC  1567 N/mm2
 460 HB  484 HV  47.9 HRC  1571 N/mm2
 461 HB  485 HV  48.0 HRC  1575 N/mm2
 462 HB  486 HV  48.1 HRC  1579 N/mm2
 463 HB  487 HV  48.2 HRC  1583 N/mm2
 464 HB  488 HV  48.3 HRC  1587 N/mm2
 465 HB  489 HV  48.3 HRC  1591 N/mm2
 466 HB  490 HV  48.4 HRC  1595 N/mm2
 467 HB  491 HV  48.4 HRC  1599 N/mm2
 468 HB  492 HV  48.5 HRC  1603 N/mm2
 469 HB  493 HV  48.5 HRC  1607 N/mm2
 470 HB  494 HV  48.6 HRC  1611 N/mm2
 471 HB  495 HV  48.7 HRC  1614 N/mm2
 472 HB  496 HV  48.8 HRC  1618 N/mm2
 473 HB  497 HV  48.9 HRC  1622 N/mm2
 474 HB  498 HV  49.0 HRC  1626 N/mm2
 475 HB  500 HV  49.1 HRC  1630 N/mm2
 476 HB  501 HV  49.2 HRC  1633 N/mm2
 477 HB  502 HV  49.2 HRC  1637 N/mm2
 478 HB  503 HV  49.3 HRC  1640 N/mm2
 479 HB  504 HV  49.4 HRC  1643 N/mm2
 480 HB  505 HV  49.5 HRC  1644 N/mm2
 481 HB  506 HV  49.5 HRC  1647 N/mm2
 482 HB  507 HV  49.6 HRC  1651 N/mm2
 483 HB  508 HV  49.7 HRC  1655 N/mm2
 484 HB  509 HV  49.7 HRC  1660 N/mm2
 485 HB  510 HV  49.8 HRC  1665 N/mm2
 486 HB  511 HV  49.9 HRC  1669 N/mm2
 487 HB  512 HV  49.9 HRC  1673 N/mm2
 488 HB  513 HV  50.0 HRC  1677 N/mm2
 489 HB  514 HV  50.1 HRC  1681 N/mm2
 490 HB  515 HV  50.2 HRC  1685 N/mm2
 491 HB  516 HV  50.3 HRC  1689 N/mm2
 492 HB  517 HV  50.3 HRC  1693 N/mm2
 493 HB  518 HV  50.4 HRC  1697 N/mm2
 494 HB  520 HV  50.5 HRC  1700 N/mm2
 495 HB  521 HV  50.5 HRC  1704 N/mm2
 496 HB  522 HV  50.6 HRC  1708 N/mm2
 497 HB  523 HV  50.6 HRC  1712 N/mm2
 498 HB  524 HV  50.7 HRC  1716 N/mm2
 499 HB  525 HV  50.7 HRC  1720 N/mm2
 500 HB  526 HV  50.8 HRC  1724 N/mm2
 501 HB  527 HV  50.8 HRC  1728 N/mm2
 502 HB  528 HV  50.9 HRC  1732 N/mm2
 503 HB  529 HV  51.0 HRC  1736 N/mm2
 504 HB  530 HV  51.1 HRC  1740 N/mm2
 505 HB  531 HV  51.1 HRC  1744 N/mm2
 506 HB  532 HV  51.2 HRC  1748 N/mm2
 507 HB  533 HV  51.2 HRC  1752 N/mm2
 508 HB  534 HV  51.3 HRC  1756 N/mm2
 509 HB  535 HV  51.4 HRC  1760 N/mm2
 510 HB  536 HV  51.5 HRC  1764 N/mm2
 511 HB  537 HV  51.5 HRC  1768 N/mm2
 512 HB  538 HV  51.6 HRC  1772 N/mm2
 513 HB  540 HV  51.7 HRC  1775 N/mm2
 514 HB  541 HV  51.7 HRC  1779 N/mm2
 515 HB  542 HV  51.8 HRC  1782 N/mm2
 516 HB  543 HV  51.8 HRC  1786 N/mm2
 517 HB  544 HV  51.9 HRC  1789 N/mm2
 518 HB  545 HV  51.9 HRC  1793 N/mm2
 519 HB  546 HV  52.0 HRC  1797 N/mm2
 520 HB  547 HV  52.0 HRC  1801 N/mm2
 521 HB  548 HV  52.1 HRC  1804 N/mm2
 522 HB  549 HV  52.2 HRC  1807 N/mm2
 523 HB  550 HV  52.3 HRC  1810 N/mm2
 524 HB  551 HV  52.3 HRC  1814 N/mm2
 525 HB  552 HV  52.4 HRC  1818 N/mm2
 526 HB  553 HV  52.4 HRC  1822 N/mm2
 527 HB  554 HV  52.5 HRC  1826 N/mm2
 528 HB  555 HV  52.6 HRC  1830 N/mm2
 529 HB  556 HV  52.7 HRC  1834 N/mm2
 530 HB  557 HV  52.8 HRC  1838 N/mm2
 531 HB  558 HV  52.9 HRC  1842 N/mm2
 532 HB  560 HV  53.0 HRC  1845 N/mm2
 533 HB  561 HV  53.0 HRC  1848 N/mm2
 534 HB  562 HV  53.1 HRC  1852 N/mm2
 535 HB  563 HV  53.1 HRC  1855 N/mm2
 536 HB  564 HV  53.2 HRC  1859 N/mm2
 537 HB  565 HV  53.2 HRC  1863 N/mm2
 538 HB  566 HV  53.3 HRC  1867 N/mm2
 539 HB  567 HV  53.3 HRC  1870 N/mm2
 540 HB  568 HV  53.4 HRC  1873 N/mm2
 541 HB  569 HV  53.5 HRC  1876 N/mm2
 542 HB  570 HV  53.6 HRC  1880 N/mm2
 543 HB  571 HV  53.6 HRC  1884 N/mm2
 544 HB  571 HV  53.7 HRC  1889 N/mm2
 545 HB  573 HV  53.7 HRC  1893 N/mm2
 546 HB  574 HV  53.8 HRC  1898 N/mm2
 547 HB  575 HV  53.8 HRC  1902 N/mm2
 548 HB  576 HV  53.9 HRC  1907 N/mm2
 549 HB  577 HV  53.9 HRC  1912 N/mm2
 550 HB  578 HV  54.0 HRC  1916 N/mm2
 551 HB  580 HV  54.1 HRC  1920 N/mm2
 552 HB  581 HV  54.1 HRC  1923 N/mm2
 553 HB  582 HV  54.2 HRC  1927 N/mm2
 554 HB  583 HV  54.2 HRC  1930 N/mm2
 555 HB  584 HV  54.3 HRC  1934 N/mm2
 556 HB  585 HV  54.3 HRC  1937 N/mm2
 557 HB  586 HV  54.4 HRC  1941 N/mm2
 558 HB  587 HV  54.4 HRC  1945 N/mm2
 559 HB  588 HV  54.5 HRC  1948 N/mm2
 560 HB  589 HV  54.6 HRC  1952 N/mm2
 561 HB  590 HV  54.7 HRC  1955 N/mm2
 562 HB  591 HV  54.7 HRC  1959 N/mm2
 563 HB  592 HV  54.8 HRC  1964 N/mm2
 564 HB  593 HV  54.8 HRC  1969 N/mm2
 565 HB  594 HV  54.9 HRC  1973 N/mm2
 566 HB  595 HV  54.9 HRC  1978 N/mm2
 567 HB  596 HV  55.0 HRC  1982 N/mm2
 568 HB  597 HV  55.1 HRC  1987 N/mm2
 569 HB  598 HV  55.1 HRC  1991 N/mm2
 570 HB  600 HV  55.2 HRC  1995 N/mm2
 571 HB  601 HV  55.2 HRC  1999 N/mm2
 572 HB  602 HV  55.3 HRC  2002 N/mm2
 573 HB  603 HV  55.3 HRC  2006 N/mm2
 574 HB  604 HV  55.4 HRC  2009 N/mm2
 575 HB  605 HV  55.4 HRC  2013 N/mm2
 576 HB  606 HV  55.5 HRC  2016 N/mm2
 577 HB  607 HV  55.5 HRC  2020 N/mm2
 578 HB  608 HV  55.6 HRC  2023 N/mm2
 579 HB  609 HV  55.6 HRC  2027 N/mm2
 580 HB  610 HV  55.7 HRC  2030 N/mm2
 581 HB  611 HV  55.7 HRC  2034 N/mm2
 582 HB  612 HV  55.8 HRC  2039 N/mm2
 583 HB  613 HV  55.8 HRC  2043 N/mm2
 584 HB  614 HV  55.9 HRC  2048 N/mm2
 585 HB  615 HV  55.9 HRC  2052 N/mm2
 586 HB  616 HV  56.0 HRC  2057 N/mm2
 587 HB  617 HV  56.1 HRC  2061 N/mm2
 588 HB  618 HV  56.2 HRC  2065 N/mm2
 589 HB  620 HV  56.3 HRC  2070 N/mm2
 590 HB  621 HV  56.3 HRC  2073 N/mm2
 591 HB  622 HV  56.4 HRC  2077 N/mm2
 592 HB  623 HV  56.4 HRC  2080 N/mm2
 593 HB  624 HV  56.5 HRC  2084 N/mm2
 594 HB  625 HV  56.5 HRC  2087 N/mm2
 595 HB  626 HV  56.6 HRC  2091 N/mm2
 596 HB  627 HV  56.6 HRC  2093 N/mm2
 597 HB  628 HV  56.7 HRC  2097 N/mm2
 598 HB  629 HV  56.7 HRC  2101 N/mm2
 599 HB  630 HV  56.8 HRC  2105 N/mm2
 600 HB  631 HV  56.8 HRC  2109 N/mm2
 601 HB  632 HV  56.9 HRC  2114 N/mm2
 602 HB  633 HV  56.9 HRC  2118 N/mm2
 603 HB  634 HV  57.0 HRC  2123 N/mm2
 604 HB  635 HV  57.0 HRC  2127 N/mm2
 605 HB  636 HV  57.1 HRC  2132 N/mm2
 606 HB  637 HV  57.2 HRC  2136 N/mm2
 607 HB  638 HV  57.2 HRC  2141 N/mm2
 608 HB  640 HV  57.3 HRC  2145 N/mm2
 609 HB  641 HV  57.3 HRC  2148 N/mm2
 610 HB  642 HV  57.4 HRC  2152 N/mm2
 611 HB  643 HV  57.4 HRC  2155 N/mm2
 612 HB  644 HV  57.5 HRC  2159 N/mm2
 613 HB  645 HV  57.5 HRC  2162 N/mm2
 614 HB  646 HV  57.6 HRC  2166 N/mm2
 615 HB  647 HV  57.6 HRC  2169 N/mm2
 616 HB  648 HV  57.7 HRC  2173 N/mm2
 617 HB  649 HV  57.7 HRC  2177 N/mm2
 618 HB  650 HV  57.8 HRC  2180 N/mm2
 - HB  651 HV  57.8 HRC  - N/mm2
 - HB  652 HV  57.8 HRC  - N/mm2
 - HB  653 HV  57.9 HRC  - N/mm2
 - HB  654 HV  57.9 HRC  - N/mm2
 - HB  655 HV  58.0 HRC  - N/mm2
 - HB  656 HV  58.0 HRC  - N/mm2
 - HB  657 HV  58.1 HRC  - N/mm2
 - HB  658 HV  58.1 HRC  - N/mm2
 - HB  660 HV  58.3 HRC  - N/mm2
 - HB  661 HV  58.3 HRC  - N/mm2
 - HB  662 HV  58.4 HRC  - N/mm2
 - HB  663 HV  58.4 HRC  - N/mm2
 - HB  664 HV  58.5 HRC  - N/mm2
 - HB  665 HV  58.5 HRC  - N/mm2
 - HB  666 HV  58.6 HRC  - N/mm2
 - HB  667 HV  58.6 HRC  - N/mm2
 - HB  668 HV  58.7 HRC  - N/mm2
 - HB  669 HV  58.7 HRC  - N/mm2
 - HB  670 HV  58.8 HRC  - N/mm2
 - HB  671 HV  58.8 HRC  - N/mm2
 - HB  672 HV  58.9 HRC  - N/mm2
 - HB  673 HV  58.9 HRC  - N/mm2
 - HB  674 HV  59.0 HRC  - N/mm2
 - HB  675 HV  59.0 HRC  - N/mm2
 - HB  676 HV  59.0 HRC  - N/mm2
 - HB  677 HV  59.1 HRC  - N/mm2
 - HB  678 HV  59.1 HRC  - N/mm2
 - HB  679 HV  59.1 HRC  - N/mm2
 - HB  680 HV  59.2 HRC  - N/mm2
 - HB  681 HV  59.2 HRC  - N/mm2
 - HB  682 HV  59.3 HRC  - N/mm2
 - HB  683 HV  59.3 HRC  - N/mm2
 - HB  684 HV  59.4 HRC  - N/mm2
 - HB  685 HV  59.4 HRC  - N/mm2
 - HB  686 HV  59.5 HRC  - N/mm2
 - HB  687 HV  59.5 HRC  - N/mm2
 - HB  688 HV  59.6 HRC  - N/mm2
 - HB  689 HV  59.6 HRC  - N/mm2
 - HB  690 HV  59.7 HRC  - N/mm2
 - HB  691 HV  59.7 HRC  - N/mm2
 - HB  692 HV  59.8 HRC  - N/mm2
 - HB  693 HV  59.8 HRC  - N/mm2
 - HB  694 HV  59.9 HRC  - N/mm2
 - HB  695 HV  59.9 HRC  - N/mm2
 - HB  696 HV  59.9 HRC  - N/mm2
 - HB  697 HV  60.0 HRC  - N/mm2
 - HB  698 HV  60.0 HRC  - N/mm2
 - HB  699 HV  60.0 HRC  - N/mm2
 - HB  700 HV  60.1 HRC  - N/mm2
 - HB  701 HV  60.1 HRC  - N/mm2
 - HB  702 HV  60.2 HRC  - N/mm2
 - HB  703 HV  60.2 HRC  - N/mm2
 - HB  704 HV  60.2 HRC  - N/mm2
 - HB  705 HV  60.3 HRC  - N/mm2
 - HB  706 HV  60.3 HRC  - N/mm2
 - HB  707 HV  60.4 HRC  - N/mm2
 - HB  708 HV  60.4 HRC  - N/mm2
 - HB  709 HV  60.5 HRC  - N/mm2
 - HB  710 HV  60.5 HRC  - N/mm2
 - HB  711 HV  60.6 HRC  - N/mm2
 - HB  712 HV  60.6 HRC  - N/mm2
 - HB  713 HV  60.7 HRC  - N/mm2
 - HB  714 HV  60.7 HRC  - N/mm2
 - HB  715 HV  60.8 HRC  - N/mm2
 - HB  716 HV  60.8 HRC  - N/mm2
 - HB  717 HV  60.8 HRC  - N/mm2
 - HB  718 HV  60.9 HRC  - N/mm2
 - HB  719 HV  60.9 HRC  - N/mm2
 - HB  720 HV  61.0 HRC  - N/mm2
 - HB  721 HV  61.0 HRC  - N/mm2
 - HB  722 HV  61.1 HRC  - N/mm2
 - HB  723 HV  61.1 HRC  - N/mm2
 - HB  724 HV  61.2 HRC  - N/mm2
 - HB  725 HV  61.2 HRC  - N/mm2
 - HB  726 HV  61.3 HRC  - N/mm2
 - HB  727 HV  61.3 HRC  - N/mm2
 - HB  728 HV  61.4 HRC  - N/mm2
 - HB  729 HV  61.4 HRC  - N/mm2
 - HB  730 HV  61.5 HRC  - N/mm2
 - HB  731 HV  61.5 HRC  - N/mm2
 - HB  732 HV  61.6 HRC  - N/mm2
 - HB  733 HV  61.6 HRC  - N/mm2
 - HB  734 HV  61.6 HRC  - N/mm2
 - HB  735 HV  61.6 HRC  - N/mm2
 - HB  736 HV  61.7 HRC  - N/mm2
 - HB  737 HV  61.7 HRC  - N/mm2
 - HB  738 HV  61.7 HRC  - N/mm2
 - HB  739 HV  61.7 HRC  - N/mm2
 - HB  740 HV  61.8 HRC  - N/mm2
 - HB  741 HV  61.8 HRC  - N/mm2
 - HB  742 HV  61.8 HRC  - N/mm2
 - HB  743 HV  61.8 HRC  - N/mm2
 - HB  744 HV  61.9 HRC  - N/mm2
 - HB  745 HV  61.9 HRC  - N/mm2
 - HB  746 HV  61.9 HRC  - N/mm2
 - HB  747 HV  62.0 HRC  - N/mm2
 - HB  748 HV  62.0 HRC  - N/mm2
 - HB  749 HV  62.0 HRC  - N/mm2
 - HB  750 HV  62.1 HRC  - N/mm2
 - HB  751 HV  62.1 HRC  - N/mm2
 - HB  752 HV  62.1 HRC  - N/mm2
 - HB  753 HV  62.2 HRC  - N/mm2
 - HB  754 HV  62.2 HRC  - N/mm2
 - HB  755 HV  62.2 HRC  - N/mm2
 - HB  756 HV  62.3 HRC  - N/mm2
 - HB  757 HV  62.3 HRC  - N/mm2
 - HB  758 HV  62.4 HRC  - N/mm2
 - HB  759 HV  62.4 HRC  - N/mm2
 - HB  760 HV  62.5 HRC  - N/mm2
 - HB  761 HV  62.5 HRC  - N/mm2
 - HB  762 HV  62.5 HRC  - N/mm2
 - HB  763 HV  62.6 HRC  - N/mm2
 - HB  764 HV  62.6 HRC  - N/mm2
 - HB  765 HV  62.6 HRC  - N/mm2
 - HB  766 HV  62.7 HRC  - N/mm2
 - HB  767 HV  62.7 HRC  - N/mm2
 - HB  768 HV  62.7 HRC  - N/mm2
 - HB  769 HV  62.8 HRC  - N/mm2
 - HB  770 HV  62.8 HRC  - N/mm2
 - HB  771 HV  62.9 HRC  - N/mm2
 - HB  772 HV  62.9 HRC  - N/mm2
 - HB  773 HV  63.0 HRC  - N/mm2
 - HB  774 HV  63.0 HRC  - N/mm2
 - HB  775 HV  63.1 HRC  - N/mm2
 - HB  776 HV  63.1 HRC  - N/mm2
 - HB  777 HV  63.1 HRC  - N/mm2
 - HB  778 HV  63.2 HRC  - N/mm2
 - HB  779 HV  63.2 HRC  - N/mm2
 - HB  780 HV  63.3 HRC  - N/mm2
 - HB  781 HV  63.3 HRC  - N/mm2
 - HB  782 HV  63.3 HRC  - N/mm2
 - HB  783 HV  63.4 HRC  - N/mm2
 - HB  784 HV  63.4 HRC  - N/mm2
 - HB  785 HV  63.4 HRC  - N/mm2
 - HB  786 HV  63.5 HRC  - N/mm2
 - HB  787 HV  63.5 HRC  - N/mm2
 - HB  788 HV  63.5 HRC  - N/mm2
 - HB  789 HV  63.6 HRC  - N/mm2
 - HB  790 HV  63.6 HRC  - N/mm2
 - HB  791 HV  63.6 HRC  - N/mm2
 - HB  792 HV  63.7 HRC  - N/mm2
 - HB  793 HV  63.7 HRC  - N/mm2
 - HB  794 HV  63.7 HRC  - N/mm2
 - HB  795 HV  63.8 HRC  - N/mm2
 - HB  796 HV  63.8 HRC  - N/mm2
 - HB  797 HV  63.8 HRC  - N/mm2
 - HB  798 HV  63.9 HRC  - N/mm2
 - HB  799 HV  63.9 HRC  - N/mm2
 - HB  800 HV  64.0 HRC  - N/mm2
 - HB  801 HV  64.1 HRC  - N/mm2
 - HB  802 HV  64.1 HRC  - N/mm2
 - HB  803 HV  64.1 HRC  - N/mm2
 - HB  804 HV  64.2 HRC  - N/mm2
 - HB  805 HV  64.2 HRC  - N/mm2
 - HB  806 HV  64.2 HRC  - N/mm2
 - HB  807 HV  64.3 HRC  - N/mm2
 - HB  808 HV  64.3 HRC  - N/mm2
 - HB  809 HV  64.3 HRC  - N/mm2
 - HB  810 HV  64.4 HRC  - N/mm2
 - HB  811 HV  64.4 HRC  - N/mm2
 - HB  812 HV  64.4 HRC  - N/mm2
 - HB  813 HV  64.4 HRC  - N/mm2
 - HB  814 HV  64.5 HRC  - N/mm2
 - HB  815 HV  64.5 HRC  - N/mm2
 - HB  816 HV  64.5 HRC  - N/mm2
 - HB  817 HV  64.6 HRC  - N/mm2
 - HB  818 HV  64.6 HRC  - N/mm2
 - HB  819 HV  64.6 HRC  - N/mm2
 - HB  820 HV  64.7 HRC  - N/mm2
 - HB  821 HV  64.7 HRC  - N/mm2
 - HB  822 HV  64.7 HRC  - N/mm2
 - HB  823 HV  64.8 HRC  - N/mm2
 - HB  824 HV  64.8 HRC  - N/mm2
 - HB  825 HV  64.8 HRC  - N/mm2
 - HB  826 HV  64.8 HRC  - N/mm2
 - HB  827 HV  64.9 HRC  - N/mm2
 - HB  828 HV  64.9 HRC  - N/mm2
 - HB  829 HV  64.9 HRC  - N/mm2
 - HB  830 HV  65.0 HRC  - N/mm2
 - HB  831 HV  65.0 HRC  - N/mm2
 - HB  832 HV  65.0 HRC  - N/mm2
 - HB  833 HV  65.0 HRC  - N/mm2
 - HB  834 HV  65.1 HRC  - N/mm2
 - HB  835 HV  65.1 HRC  - N/mm2
 - HB  836 HV  65.1 HRC  - N/mm2
 - HB  837 HV  65.2 HRC  - N/mm2
 - HB  838 HV  65.2 HRC  - N/mm2
 - HB  839 HV  65.2 HRC  - N/mm2
 - HB  840 HV  65.3 HRC  - N/mm2
 - HB  841 HV  65.3 HRC  - N/mm2
 - HB  842 HV  65.3 HRC  - N/mm2
 - HB  843 HV  65.4 HRC  - N/mm2
 - HB  844 HV  65.4 HRC  - N/mm2
 - HB  845 HV  65.4 HRC  - N/mm2
 - HB  846 HV  65.5 HRC  - N/mm2
 - HB  847 HV  65.5 HRC  - N/mm2
 - HB  848 HV  65.5 HRC  - N/mm2
 - HB  849 HV  65.5 HRC  - N/mm2
 - HB  850 HV  65.6 HRC  - N/mm2
 - HB  851 HV  65.6 HRC  - N/mm2
 - HB  852 HV  65.6 HRC  - N/mm2
 - HB  853 HV  65.7 HRC  - N/mm2
 - HB  854 HV  65.7 HRC  - N/mm2
 - HB  855 HV  65.7 HRC  - N/mm2
 - HB  856 HV  65.8 HRC  - N/mm2
 - HB  857 HV  65.8 HRC  - N/mm2
 - HB  858 HV  65.8 HRC  - N/mm2
 - HB  859 HV  65.9 HRC  - N/mm2
 - HB  860 HV  65.9 HRC  - N/mm2
 - HB  861 HV  65.9 HRC  - N/mm2
 - HB  862 HV  65.9 HRC  - N/mm2
 - HB  863 HV  66.0 HRC  - N/mm2
 - HB  864 HV  66.0 HRC  - N/mm2
 - HB  865 HV  66.0 HRC  - N/mm2
 - HB  866 HV  66.0 HRC  - N/mm2
 - HB  867 HV  66.1 HRC  - N/mm2
 - HB  868 HV  66.1 HRC  - N/mm2
 - HB  869 HV  66.1 HRC  - N/mm2
 - HB  870 HV  66.1 HRC  - N/mm2
 - HB  871 HV  66.2 HRC  - N/mm2
 - HB  872 HV  66.2 HRC  - N/mm2
 - HB  873 HV  66.2 HRC  - N/mm2
 - HB  874 HV  66.2 HRC  - N/mm2
 - HB  875 HV  66.3 HRC  - N/mm2
 - HB  876 HV  66.3 HRC  - N/mm2
 - HB  877 HV  66.3 HRC  - N/mm2
 - HB  878 HV  66.3 HRC  - N/mm2
 - HB  879 HV  66.4 HRC  - N/mm2
 - HB  880 HV  66.4 HRC  - N/mm2
 - HB  881 HV  66.4 HRC  - N/mm2
 - HB  882 HV  66.4 HRC  - N/mm2
 - HB  883 HV  66.5 HRC  - N/mm2
 - HB  884 HV  66.5 HRC  - N/mm2
 - HB  885 HV  66.5 HRC  - N/mm2
 - HB  886 HV  66.5 HRC  - N/mm2
 - HB  887 HV  66.5 HRC  - N/mm2
 - HB  888 HV  66.6 HRC  - N/mm2
 - HB  889 HV  66.6 HRC  - N/mm2
 - HB  890 HV  66.6 HRC  - N/mm2
 - HB  891 HV  66.7 HRC  - N/mm2
 - HB  892 HV  66.7 HRC  - N/mm2
 - HB  893 HV  66.7 HRC  - N/mm2
 - HB  894 HV  66.7 HRC  - N/mm2
 - HB  895 HV  66.8 HRC  - N/mm2
 - HB  896 HV  66.8 HRC  - N/mm2
 - HB  897 HV  66.8 HRC  - N/mm2
 - HB  898 HV  66.9 HRC  - N/mm2
 - HB  899 HV  66.9 HRC  - N/mm2
 - HB  900 HV  67.0 HRC  - N/mm2
 - HB  901 HV  67.0 HRC  - N/mm2
 - HB  902 HV  67.0 HRC  - N/mm2
 - HB  903 HV  67.0 HRC  - N/mm2
 - HB  904 HV  67.0 HRC  - N/mm2
 - HB  905 HV  67.1 HRC  - N/mm2
 - HB  906 HV  67.1 HRC  - N/mm2
 - HB  907 HV  67.1 HRC  - N/mm2
 - HB  908 HV  67.1 HRC  - N/mm2
 - HB  909 HV  67.2 HRC  - N/mm2
 - HB  910 HV  67.2 HRC  - N/mm2
 - HB  911 HV  67.2 HRC  - N/mm2
 - HB  912 HV  67.2 HRC  - N/mm2
 - HB  913 HV  67.2 HRC  - N/mm2
 - HB  914 HV  67.3 HRC  - N/mm2
 - HB  915 HV  67.3 HRC  - N/mm2
 - HB  916 HV  67.3 HRC  - N/mm2
 - HB  917 HV  67.4 HRC  - N/mm2
 - HB  918 HV  67.4 HRC  - N/mm2
 - HB  919 HV  67.4 HRC  - N/mm2
 - HB  920 HV  67.5 HRC  - N/mm2
 - HB  921 HV  67.5 HRC  - N/mm2
 - HB  921 HV  67.5 HRC  - N/mm2
 - HB  923 HV  67.5 HRC  - N/mm2
 - HB  924 HV  67.6 HRC  - N/mm2
 - HB  925 HV  67.6 HRC  - N/mm2
 - HB  926 HV  67.6 HRC  - N/mm2
 - HB  927 HV  67.6 HRC  - N/mm2
 - HB  928 HV  67.7 HRC  - N/mm2
 - HB  929 HV  67.7 HRC  - N/mm2
 - HB  930 HV  67.7 HRC  - N/mm2
 - HB  931 HV  67.7 HRC  - N/mm2
 - HB  932 HV  67.8 HRC  - N/mm2
 - HB  933 HV  67.8 HRC  - N/mm2
 - HB  934 HV  67.8 HRC  - N/mm2
 - HB  935 HV  67.8 HRC  - N/mm2
 - HB  936 HV  67.9 HRC  - N/mm2
 - HB  937 HV  67.9 HRC  - N/mm2
 - HB  938 HV  67.9 HRC  - N/mm2
 - HB  939 HV  67.9 HRC  - N/mm2
 - HB  940 HV  68.0 HRC  - N/mm2