Ni-Mn alloys - Electrolytic polishing

Material Name: Ni-Mn alloys
Recipe No.: 4186
Primary Chemical Element in Material: Ni
Sample Type: Bulk
Uses: Electrolytic polishing
Etchant Name: None
Type (Macro/Micro): Micro
Etching Method: Electrolytic polishing
Etchant (Electrolyte) Composition: 100 ccs phosphoric acid, 100 ccs ethyl alcohol.
Procedure (Condition): Cathode: Cu plate of large area, CD: 2 A/cm2, temperature: 40 C, time: 2 mins.
Note: No data
Reference: T.Taoka, et al., J.Phys.Soc.Jap., Vol.11, No.5, May 1956, p. 522.