Molybdenum - Electrolytic thinning

Material Name: Molybdenum
Recipe No.: 4215
Primary Chemical Element in Material: Mo
Sample Type: Thin foil
Uses: Electrolytic thinning
Etchant Name: None
Type (Macro/Micro): Micro
Etching Method: Electrolytic thinning
Etchant (Electrolyte) Composition: 93% sulphuric acid, 7% water.
Procedure (Condition): CD: 0.8-1.0 A/cm2, temperature: 50 C.
Note: No data
Reference: P.R.B.Higgins, et al., J.Less Comm.Metals, Vol.6, 1964, p. 472.