Carbon and alloy steel specimens - Segregation, porosity, hardness penetration, cracks

Material Name: Carbon and alloy steel
Recipe No.: 617
Primary Chemical Element in Material: Fe
Sample Type: Bulk
Uses: Segregation, porosity, hardness penetration, cracks
Etchant Name: None
Type (Macro/Micro): Macro
Etching Method: Chemical
Etchant (Electrolyte) Composition: Concentrated HCl.
Procedure (Condition): 15-60 min, 71-82 C (160-180 F).
Note: Segregation, porosity, hardness penetration, cracks, inclusions, dendrites, flow lines, soft spots, structure, weld examination. Saw-cut or machined surface or average ground surface of sample.
Reference: Metallography, Structures and Phase Diagrams, Metals Handbook, 8th Edition, Vol. 8, ASM (American Society for Metals), Metals Park, Ohio 44079, USA, 1973, p. 71.