Ni and Ni alloys - Electrolytic polishing

Material Name: Ni and Ni alloys
Recipe No.: 9982
Primary Chemical Element in Material: Ni
Sample Type: Bulk
Uses: Polishing
Etchant Name: None
Type (Macro/Micro): Micro
Etching Method: Electrolytic polishing
Etchant (Electrolyte) Composition: 10 ml perchloric acid, 90 ml acetic acid.
Procedure (Condition): Current density: 8-12 A/cm2, time: 30-90 s.
Note: Used for Inconel X. Begelow and coworkers.
Reference: Vander Voort, Metallography Principles and Practice, McGraw-Hill, Inc., 1984, p. 587.